Procedure for Etching Copper

Etching Copper off Nickel

After mounting the target on a frame (e.g. epoxy) prepare the target for etching by dipping it in trichloroethylene – UN1710, a degreaser. Next prepare the solution:

75 mL of 23% Ammonium Hydroxide – UN2672 (NH4OH)
25 mL 50% H2O2.

Dip the foil in the solution and a blue discoloration will immediately appear, see picture. Remove after bubbling has ceased. If the solution bubbles over, use less hydrogen peroxide. Dip the foil again in trichloroethylene .

Dip the foil in the solution and a blue discoloration will immediately appear Remove the foil after bubbling has ceased

1.0 MeV Protons Backscattered (165 degrees) off the nickel foil.
1.0 MeV Protons Backscattered (165 degrees) off the nickel foil.

Tristan and Moshe discussing the procedure for etching Copper off of Nickel.

Tristan and Moshe discussing the procedure for etching Copper off of Nickel.